Choosing Materials for Permanent Magnets, Electromagnets and Transformer Cores
This chapter assumes you know the hysteresis loop (B against H), the terms retentivity and coercivity, and the relations B = μ0(H + M), χ = M/H and μr = 1 + χ. It uses them to answer a practical question: given a job, which ferromagnetic material should you pick?
The selection problem
All three applications use a ferromagnetic material, but they ask for opposite things from its hysteresis loop.
- A permanent magnet must keep its magnetization after the field that created it is removed, and must resist being demagnetized by stray fields.
- An electromagnet must magnetize strongly when the current is on and lose almost all magnetism when the current is off.
- A transformer core is magnetized and demagnetized many times per second. It must do this with as little wasted energy as possible.
The loop's shape tells you which job a material suits. Three features matter most.
| Loop feature | Meaning | Where it shows |
|---|---|---|
| Retentivity (remanence) | B left in the material when H returns to zero | Height of the loop where it crosses the B axis |
| Coercivity | Reverse H needed to bring B to zero | Width of the loop where it crosses the H axis |
| Loop area | Energy lost as heat per unit volume per cycle | Area enclosed by the loop |
A fourth property is permeability. A high μr means a small H produces a large B, so a small current in the coil gives a strong field.
Permanent magnets
A permanent magnet needs both high retentivity and high coercivity. High retentivity gives a strong field. High coercivity keeps that field from being erased by heat, vibration or a nearby opposing field. The loop is therefore wide and tall. Its large area does not matter, because the magnet is magnetized once and never cycled.
Typical materials:
- Steel (carbon steel) and alnico, an alloy of aluminium, nickel, cobalt and iron, have high retentivity and high coercivity.
- Modern rare-earth alloys such as neodymium-iron-boron and samarium-cobalt have even larger coercivity and make very strong magnets.
- Soft iron is a poor choice. Its coercivity is low, so a small reverse field or a knock removes most of its magnetism.
A standard NEET point is that steel is preferred over soft iron for permanent magnets, even though soft iron has higher permeability and is magnetized more easily. Steel is harder to magnetize but keeps the magnetism. Soft iron is easy to magnetize and easy to demagnetize.
Electromagnets
An electromagnet is a coil, often a solenoid, wound around a ferromagnetic core. The core multiplies the field of the coil by about μr. The field is only wanted while the current flows. The core should have:
- High permeability and high saturation magnetization, so a modest current gives a strong field.
- Low retentivity, so the field nearly vanishes when the current is switched off.
- Low coercivity, so the core is demagnetized by a small reverse field and follows the coil current easily.
This describes a soft magnetic material, with a narrow, tall, steep loop. Soft iron is the standard answer. Other examples are mumetal and permalloy (nickel-iron alloys) and silicon steel.
The narrow loop has a second benefit. Because the area is small, little heat is generated when the current changes direction.
Transformer cores and other AC devices
A transformer core is driven by an alternating current. At 50 Hz, the material traces its whole hysteresis loop 50 times every second. The energy lost per cycle is proportional to the loop area, so the total power lost as heat is proportional to the loop area times the frequency. The core must therefore have a very small loop area.
Two kinds of loss matter.
- Hysteresis loss. This is the energy dissipated in reorienting magnetic domains around the loop. It is reduced by choosing a material with a narrow loop: low coercivity and low retentivity. Silicon steel is the usual choice. Adding a few percent of silicon to iron narrows the loop and also raises the electrical resistivity.
- Eddy current loss. The changing flux induces circulating currents inside the core itself. These currents heat the core. The loss is reduced in two ways. A higher resistivity (silicon steel again) makes the currents smaller. Building the core from thin laminations, which are sheets insulated from each other by varnish or oxide, breaks the paths the currents would follow.
The same logic applies to the cores of AC motors and generators, and to chokes. All of them cycle the core repeatedly, so all use soft, laminated material.
Eddy currents are not part of the hysteresis loop. A material can have a narrow loop and still run hot in a solid block, because the loop only accounts for hysteresis loss.
Comparison summary
| Property | Permanent magnet | Electromagnet core | Transformer core |
|---|---|---|---|
| Retentivity | High | Low | Low |
| Coercivity | High | Low | Low |
| Permeability | Not the main concern | High | High |
| Loop area | Large, acceptable | Small | Very small |
| Typical material | Steel, alnico, NdFeB | Soft iron | Laminated silicon steel |
| Magnetization during use | Constant | On and off with current | Reverses every half cycle |
Common errors
- Confusing "easy to magnetize" with "good permanent magnet". Soft iron magnetizes easily but loses the magnetism. Ease of magnetization (high μr) is a requirement for electromagnet cores. It is not a requirement for permanent magnets.
- Mixing up retentivity and coercivity. Retentivity is how much B remains at H = 0. Coercivity is how much reverse H is needed to remove it. A permanent magnet needs both to be high. A soft core needs both to be low.
- Forgetting eddy currents. Lamination does not change the hysteresis loop. It cuts a separate loss.
- Assuming a large loop area is always bad. It is bad when the material is cycled. It is irrelevant for a magnet that is magnetized once.
- Using a ferromagnet above its Curie temperature. Above the Curie temperature, a ferromagnet turns paramagnetic and follows the Curie-Weiss law. A permanent magnet heated past this point loses its magnetization, so a magnet for hot service needs a high Curie temperature as well as high coercivity.
Worked example: comparing the heat produced
A soft iron core and a steel core are each taken around a full hysteresis loop at 50 Hz. The loop areas are 200 J m⁻³ per cycle for steel and 20 J m⁻³ per cycle for soft iron. The core volume is 2.0 × 10⁻³ m³ in each case. Find the power lost to hysteresis in each.
Energy lost per cycle is the loop area times the volume. Power is that energy times the frequency.
The following code carries out the calculation.
def hysteresis_power(loop_area, volume, frequency):
# loop_area in J per m^3 per cycle, volume in m^3, frequency in Hz
return loop_area * volume * frequency
volume = 2.0e-3
frequency = 50
steel = hysteresis_power(200, volume, frequency)
soft_iron = hysteresis_power(20, volume, frequency)
print(f"Steel core: {steel:.1f} W")
print(f"Soft iron core: {soft_iron:.1f} W")
print(f"Ratio: {steel / soft_iron:.0f}")The output is 20.0 W for steel and 2.0 W for soft iron, a ratio of 10. The steel core, with ten times the loop area, loses ten times as much power. This is why steel makes a poor transformer core and a good permanent magnet, while soft iron does the reverse.
Linking to earlier chapters
The choice of material connects to the earlier ideas in this tutorial.
- Susceptibility is large and positive for ferromagnets, so μr = 1 + χ is much greater than 1. This is why a core multiplies the coil's field.
- Domains explain the loop. In soft materials, domain walls move easily, so the loop is narrow. In hard materials, the walls are pinned by impurities and strain, so the loop is wide.
- The Curie temperature sets an upper limit on the working temperature of every material in this chapter.
Exercise
A material has a very narrow hysteresis loop with a steep slope near the origin and low retentivity. (a) State one use for it and one use for which it is unsuitable. (b) Explain both answers.
Show answer
(a) It suits an electromagnet core or a transformer core. It is unsuitable for a permanent magnet. (b) The steep slope means high permeability, so a small H gives a large B. Low retentivity and low coercivity mean the magnetism disappears when the field is removed, and the small loop area means little energy is lost per cycle. These properties are what an electromagnet or transformer needs. A permanent magnet needs the opposite: high retentivity to hold a strong field and high coercivity to resist demagnetization.
Exercise
A transformer core is built from many thin sheets of silicon steel insulated from each other, rather than from a solid block of the same alloy. Which loss does the lamination reduce, and why does the silicon content help with both losses?
Show answer
Lamination reduces eddy current loss, because the insulation between sheets breaks up the paths for the currents induced by the changing flux. Silicon narrows the hysteresis loop, which reduces hysteresis loss. Silicon also raises the electrical resistivity, which makes the eddy currents smaller.
Exercise
A core with a loop area of 50 J m⁻³ per cycle and volume 1.0 × 10⁻³ m³ is used at 60 Hz. Find the hysteresis power loss.
Show answer
Energy lost per cycle = 50 × 1.0 × 10⁻³ = 0.05 J. Power = 0.05 × 60 = 3 W.